Gear Surface Treatments: Shot Peening, Superfinishing and Coatings Compared
Heat treatment and hard finishing set a gear's core properties and tooth geometry. Surface treatments come after them and change only a thin outer layer, yet that layer is where many gear failures begin. Shot peening, superfinishing and coatings each act on a different failure mode, so the right choice depends on how the gear is expected to fail.
This guide compares the three for design engineers and sourcing teams. It covers what each treatment does, where it sits in the process route, and what the drawing has to say about it. Many shops send one or more of these steps to specialist sources. An RFQ should therefore ask any supplier which steps it performs in-house, which it subcontracts, and under which accreditation.
Start From the Failure Mode
Gear teeth fail in a few recognizable ways. Bending fatigue starts at the root fillet, where tensile stress peaks as each tooth is loaded. Surface fatigue appears on the active flank as micropitting or pitting. Scuffing and adhesive wear occur when sliding contact outruns the lubricant film.
Each treatment targets part of that list. Shot peening works on the root. Superfinishing works on the flank surface. Coatings change friction and wear behavior at the contact itself. Choosing a treatment before naming the failure mode it should prevent is a common way to add cost without adding life.
| Treatment | Main purpose | Failure mode addressed | What changes on the part | Typical position in the route |
|---|---|---|---|---|
| Shot peening | Compressive residual stress in the surface layer | Root bending fatigue | Surface texture roughens; selected areas may be masked | After the last grinding of the peened area |
| Superfinishing | Lower flank roughness | Micropitting, pitting, scuffing; friction and noise | Very small stock removal; profile and lead are re-checked | After grinding or honing, and after peening |
| Black oxide | Appearance and handling protection | Light corrosion during storage | Negligible build | Final step |
| Manganese phosphate | Oil retention during run-in | Galling and scuffing at break-in | Converted surface layer | Final step |
| Thin-film PVD (DLC, WC/C) | Hard, low-friction film | Scuffing, wear, surface fatigue under marginal lubrication | Thin film added to finished flanks | Final step, after all finishing |

Shot Peening: Compressive Stress Where Roots Crack
Shot peening bombards the surface with spherical media made of metal, glass or ceramic. Each impact plastically deforms a small area and leaves a thin layer in residual compression. At the tooth root, that compression offsets part of the tensile bending stress that drives fatigue cracks.
The American Gear Manufacturers Association describes the process in AGMA 938-A05, Shot Peening of Gears. The document is an information sheet, and it deliberately avoids quantifying rating increases from peening. It states that any rating increase credited to shot peening should be agreed between the gear manufacturer and the purchaser, and preferably verified through testing.
Intensity and coverage
Peening is controlled by intensity and coverage. Intensity is measured on Almen test strips, which bow when peened on one side. SAE J442 defines the strip, holder and gage, and SAE J443 describes how to use them, including saturation curves. Coverage expresses how much of the target surface has been impacted.
Aerospace drawings often call up SAE AMS2430 for automatic shot peening, or AMS2432 for computer-monitored peening. AMS2432 builds on the AMS2430 requirements and adds real-time monitoring of process inputs.
Effects on the flank
Peening roughens the surface it treats. On the active flank, that roughness can work against surface durability even as the root gains bending strength. Programs therefore often peen the roots and mask the flanks, or they add a finishing step after peening. Grinding a peened area afterwards removes part of the compressive layer, so the sequence belongs on the drawing.
Shot peening is a special process on many aerospace programs. Buyers should confirm that a supplier's accreditation scope covers peening itself, because an accreditation for another special process does not extend to it. Batom performs shot peening in-house under its own Nadcap accreditation, listed on its Manufacturing Spec page under Surface Enhancement (checklist AC7117/2).
With grinding and peening in the same plant, the sequencing problem above can be settled at the drawing stage. Batom's engineers agree the masking plan and the grind-then-peen order with the customer during the DFM review, before the first sample is cut.
Superfinishing: Lower Roughness on the Active Flank
Superfinishing reduces flank roughness after grinding or honing. A common industrial form is chemically accelerated vibratory finishing. A mild chemistry forms a soft layer on the surface, and vibratory media remove that layer from the peaks first. Repeating the cycle levels the asperities while the valleys are largely untouched.
NASA has measured what superfinishing does to gear life. In NASA Technical Memorandum 2000-210044, Krantz and co-authors tested case-carburized AISI 9310 spur gears finished in a vibrated bed of zinc chips, water and aluminum oxide powder. Superfinishing reduced the roughness average by about a factor of five. At 1.71 GPa Hertz contact stress, the superfinished gears lived about four times longer than ground gears of otherwise similar quality. The report attributes that difference to the combined effects of the different tooth surface topography and the two gear sets coming from different melts of steel.
Superfinishing removes very little material, but it still touches the flank. Intended micro-geometry such as tip relief and crowning has to survive the process, so profile and lead should be measured again afterwards. Surface finish also affects gear noise, which is one reason noise-sensitive programs consider it. Batom performs superfinishing in-house, so the finishing step and the profile and lead re-measurement after it stay under one roof.
Honing is a related but separate route. Batom's manufacturing page, which lists two Fässler HMX-400 power honing machines, describes power honing as producing "an excellent surface – free from grinding burn". The same page says honed gears "produce less noise and have a longer use life". Batom's gear NVH FAQ also notes that grinding and power honing can improve the surface structure. The drawing should state which finishing route it requires.
Coatings: Film Thickness Is a Tolerance Decision
Coatings range from conversion layers with almost no build to thin hard films. Every option carries the same drawing requirement: state whether the tooth dimensions apply before or after coating.
Black oxide
Black oxide is a conversion coating for ferrous metals, specified in the US under MIL-DTL-13924. The specification notes that it offers only very limited corrosion protection under mildly corrosive conditions, even with a supplementary preservative. It suits appearance and handling protection. It is not a wear or fatigue treatment.
Manganese phosphate
Heavy phosphate coatings are specified under MIL-DTL-16232, which covers manganese and zinc types applied by immersion. Manganese phosphate is widely used to reduce galling and improve break-in of sliding steel surfaces. The porous layer holds oil, and most of its corrosion resistance comes from that supplementary oil.
Thin-film PVD: DLC and WC/C
Carbon-based films are classified in ISO 20523:2017, which includes amorphous carbon films commonly called diamond-like carbon. Metal-containing variants such as WC/C are typically deposited by sputtering.
NASA tested one such film on gears. NASA Technical Memorandum 2003-212463 applied a metal-containing, carbon-based coating to case-carburized AISI 9310 spur gears. The report describes approximately a six-fold increase in surface fatigue life. All 15 uncoated tests failed before 275 million revolutions, while 11 of 14 coated tests were suspended without failure.
Two limits apply. The deposition temperature must stay compatible with the tempering condition of the hardened case. The substrate must also be hard enough to support a thin film under contact load.
Electroplated coatings and hydrogen
Electroplating high-strength steel introduces a risk of hydrogen embrittlement. ASTM B850 describes post-coating heat treatments that reduce that risk. It also notes that these treatments do not guarantee complete freedom from hydrogen degradation. For case-hardened gears, the relief treatment has to be agreed against the part's heat treatment.
Batom completes coatings through certified supply-chain partners and schedules the coating step inside the same route as its grinding, peening and inspection. On the Nadcap list of Batom's Manufacturing Spec page, the dry film lubricant coating, chrome plating and passivation entries are those partners' accreditations. For each coating, the certificate to check is the one held by the facility that applies it.
Where Each Treatment Sits in the Route
Sequence decides whether a treatment keeps its benefit. A route that is commonly used, and always confirmed against the drawing, runs as follows:
- Heat treatment of the gear
- Hard finishing by grinding or power honing
- Grinding burn inspection after the last grinding operation
- Shot peening of the roots, with flanks masked as specified
- Superfinishing of the flanks where required
- Coating as the final surface step
- Final dimensional and gear inspection
Peening and coating parameters are chosen against the hardened case, so the heat treatment route has to be settled first.
For a closer look at how carburizing, nitriding and induction hardening form the hardened case, see the heat treatment comparison.

Specifying Surface Treatments on the Drawing
A surface treatment callout needs the same precision as a tolerance callout. The table lists what each one should state.
| Treatment | What to state on the drawing | How it is verified |
|---|---|---|
| Shot peening | Specification (for example AMS2430 or AMS2432), media type and size, intensity range, coverage, areas to peen and to mask | Almen strip records, coverage inspection |
| Superfinishing | Roughness parameter and limit, maximum stock removal, requirement to re-measure profile and lead | Roughness trace, gear measurement after finishing |
| Black oxide or phosphate | Specification and class or type, supplementary oil, whether dimensions apply before or after coating | Visual inspection and the checks the specification requires |
| Thin-film PVD | Film type, thickness range, coated areas, maximum process temperature | Thickness and adhesion checks agreed with the supplier |
| Electroplating | Plating specification and hydrogen embrittlement relief | Relief treatment records |
State surface hardness, core hardness and effective case depth as ranges, because peening and coating parameters are selected against them. All specifications customizable per customer requirements & gear specifications.
Questions to Ask a Supplier
For each treatment on the drawing, ask who performs it and under which accreditation. Nadcap accredits by special process category, so check the category for each step. Batom runs its own Nadcap-accredited magnetic particle inspection and shot peening in-house, along with superfinishing, and completes heat treatment and coatings with tightly integrated, certified supply-chain partners.
The Nadcap supplier qualification guide covers how to search and verify an accreditation in more depth than this section allows.
Ask how the treated gear is inspected afterwards. Profile, lead and pitch should be re-measured on a gear measuring machine whenever a step touches the flank. Batom's published inspection equipment includes Klingelnberg P-26, P-40 and P-65 gear measuring centers and a Frenco ZWP 06/14/24 gear rolling tester.
Batom publishes its own inspection and abrasive flow services separately. Its commissioned inspection services list magnetic particle inspection, grinding burn inspection and particle cleanliness inspection, together with abrasive flow machining, abrasive flow polishing and abrasive flow deburring. Its abrasive flow FAQ explains how a viscoelastic abrasive medium reaches internal features that tools cannot. Batom's grinding burn inspection conforms to AMS2649, and its Nadcap-accredited magnetic particle inspection follows ASTM E1444. The gear design and analysis work covers grinding notch analysis, profile and lead modifications, and transmission error.
Sources
- NASA TM-2000-210044: Surface Fatigue Lives of Case-Carburized Gears With an Improved Surface Finish
- NASA TM-2003-212463: Increased Surface Fatigue Lives of Spur Gears by Application of a Coating
- SAE AMS2430: Shot Peening
- SAE J442: Test Strip, Holder, and Gage for Shot Peening
- AGMA 938-A05: Shot Peening of Gears
About the Author
Batom Co., Ltd. Marketing Department
Batom Co., Ltd. was founded in 1981 and is headquartered in Dali District, Taichung. It has over 40 years in gear manufacture and inspection as a Leading Precision Gear Manufacturer. It provides a one-stop custom service for core gear components, built to the customer's drawing, from early DFM co-development through series production and after-sales support. From the gear manufacturing side, the drawing is where a surface treatment callout succeeds or fails. A callout that names the treatment but leaves out the sequence, the masked areas, or whether dimensions apply before or after it leaves every supplier in the route to guess. Writing the callout backwards from the failure mode closes those gaps before the RFQ goes out.
Whether you are prototyping a new gear or scaling up series production, send the drawing to Batom's engineering team with the failure mode you are designing against. The review covers the whole route for the gear components, from the grind-then-peen order to the inspection after each finishing step. An early design is enough to start the DFM discussion, and the RFQ can still ask for the accreditation behind each special process. Batom builds to your drawing and does not sell standard catalog gears or reducers.
Frequently Asked Questions
Q: What does shot peening do to a gear? A: Shot peening impacts the surface with spherical media and leaves a thin layer of compressive residual stress. At the tooth root, that stress helps resist bending fatigue cracks. AGMA 938-A05 states that any rating increase credited to peening should be agreed between the gear manufacturer and the purchaser, and preferably verified through testing.
Q: Does superfinishing improve gear fatigue life? A: It can. In NASA Technical Memorandum 2000-210044, superfinishing reduced the roughness average of case-carburized AISI 9310 spur gears by about a factor of five. At 1.71 GPa Hertz contact stress, those gears lived about four times longer than ground gears of otherwise similar quality. NASA attributes the difference to the combined effects of the superfinished surface topography and the use of different steel melts.
Q: Can a coating extend gear surface fatigue life? A: It can under test conditions. NASA Technical Memorandum 2003-212463 applied a metal-containing, carbon-based coating to case-carburized AISI 9310 spur gears and reported approximately a six-fold increase in surface fatigue life. Deposition temperature and film thickness must be checked against the gear's heat treatment and tolerances.
Q: Should gears be shot peened before or after grinding? A: Peening is commonly applied after the last grinding operation on the peened area, because later grinding removes part of the compressive layer. Peening also roughens the surface, so flanks are often masked or finished afterwards. The sequence should be written on the drawing and agreed with the supplier.
Q: What is manganese phosphate coating used for on gears? A: Heavy manganese phosphate, specified under MIL-DTL-16232, is a conversion coating that holds oil. It is widely used to reduce galling and improve break-in of sliding steel surfaces. Most of its corrosion resistance comes from the supplementary oil it retains.